Page 5 - MENDERES KATALOG - ENG
P. 5

CLOTH SPREADING                  thorn apart, if the dispersion of  •If the effusion is over the fusible
                                              the coating powder remained on  interlining, reduce the tempera-
             The spread part should be free of   the base cloth is not homoge-  ture of the press upper resist-
             humidity. If the cloth of the fusible   neous,  then  the  press cylinders  ance.
             interlining is laid for a long time   might have corroded.
             after spreading, high humidity of                                • Decrease the pressure.
             them may cause negative effects.   • Do the fusing application in dif-
             In such cases, firstly by com-   ferent  parts  of  the  press.  If  you  • Increase the speed.
             pressing separately, the humid-  end in varied results, contact with
             ity  should be removed. With this   the press machine manufacturer   4. Bad fusing and bad handle af-
             method, the cloths have a sort   or the technical service.       ter the application
             of sanforizing even they have not
             been finished as so.             2. Bowing because of shrinkage   •In this case, it means that, be-
                                                                              cause of the over heat and the low
             BONDING QUALITY                  • Compress the cloth. Check the  pressure, the coat was separated
             CONTROL AND LAST                 shrinkage difference with anoth-  from the fusible interlining but
             IRON                             er cloth, cut in the same dimen-  was not transferred to the cloth
                                              sions.                          successfully. Thus, the coat be-
             At  the  testing  stage,  do  not  go                            comes a hard layer between the
             into  the  bulk  production  with-  •If  there  is  no  problem  with  the  cloth and the interlining and with-
             out  checking  the  dismantle-   cloth, fuse the interlining with  out fusing to the cloth, it worsens
             ment  strength.  The  detachment   the compressed cloth, and check  the handle.
             strength after fusing, for the cloth   the shrinkage difference with an-
             and  fusible  interlining,  cut  and   other interlining, cut in the same  5.If risings occur on the shirt after
             fused as 5cm width stripes should   dimensions. If the shrinkage  washing then it means
             ast 1.2kg. During dismantlement,   against heat exceeds the stand-
             remember  that  some  portion  of   ards, contact to the related per-  •The press compression is low;
             the  coat  of  the  fusible  interlin-  son from the help desk.      coat  transfer  is  not at  the  ade-
             ing must remain on the contrary                                  quate level.
             applied  cloth.  Do  not  exceed  the   3. Effusion of the coat over the
             temperature of 160 degrees Cel-  cloth or fusible interlining    •The press speed is too high and
             sius  while  ironing  the  shirt  as                             the fusing is not reliable.
             approaching to the melting tem-  • If the effusion is over the cloth,
             perature  of  the  coat  may  risk   reduce the temperature of the  •The press temperature is too
             the  fusing  application.  Wash  the   press lower resistance.   low and the fusing is not reliable.
             fused shirts 5 times at 90 degrees
             Celsius and check whether there   • After that decrease the pres-  •The interlining coat level is low
             is pilling on the surface of adhe-  sure and increase the speed.   and the fusing is not reliable.
             sion or not.

             POSSIBLE PROBLEMS
             DURING APPLICATION
             AND
             TROUBLESHOOTING


             1. If the fusing is unbalanced


             • When the fusible interlining is
   1   2   3   4   5   6   7   8   9   10